| S.No. | Atribut | Unit | Chemshun 92 | Chemshun 92 | Chemshun 95 | Chemshun ZTA |
| 1 | Eusi Alumina | % | 92 | 92 | 95 | 70-75 |
| ZrO2 | % | 25-30 | ||||
| 3 | Kapadetan | g/cc | ≥3.60 | ≥3.60 | >3.65 | ≥4.2 |
| 4 | Warna | - | Bodas | Bodas | Bodas | Bodas |
| 5 | Nyerep Cai | % | <0.01 | <0.01 | 0 | 0 |
| 6 | Kakuatan Fléksibel | Mpa | 270 | 300 | 320 | 680 |
| 7 | Kapadetan Moh | Kelas | 9 | 9 | 9 | 9 |
| 8 | Karasa Sumur Batu | HRA | 80 | 85 | 87 | 90 |
| 9 | Karasa Vickers (HV5) | Kg/mm2 | 1000 | 1150 | 1200 | 1300 |
| 10 | Kateguhan Retakan (Min) | MPa.m1/2 | 3-4 | 3-4 | 3-4 | 4-5 |
| 11 | Kakuatan komprési | Mpa | 850 | 850 | 870 | 1500 |
| 12 | Koefisien Ékspansi Termal (25-1000 ℃) | 1×10-6/℃ | 8 | 7.6 | 8.1 | 8.3 |
| 13 | Suhu operasi maksimum | ℃ | 1450 | 1450 | 1500 | 1500
|